Go to the aluSelect Home Page Physical and Elastic Properties
Wrought Alloys
------------------
Casting Alloys

Go to aluMATTER Website...

Alloys:

EN AW-1050A / ISO Al99,5
Temper Elastic Physical
E
G
ν
Tsol
Tliq
Cp
α
ρ
ρel
λ
EC
MPa
MPa
°C
°C
J kg-1 K-1
µm m-1 K-1
kg m-3
nΩ m
W m-1 K-1
%IACS
69000
25900
0.33
645
658
899
23.5
2700
29
229
59.5
69000
25900
0.33
645
658
899
23.5
2700
29
229
59.5
69000
25900
0.33
645
658
899
23.5
2700
29
229
59.5
69000
25900
0.33
645
658
899
23.5
2700
29
229
59.5
69000
25900
0.33
645
658
899
23.5
2700
29
229
59.5
69000
25900
0.33
645
658
899
23.5
2700
 

 

 
Key to Parameters:
E  Modulus of elasticity  MPa
G  Modulus of rigidity  MPa
ν  Poisson's ratio 
Tsol  Solidus temperature  °C
Tliq  Liquidus temperature  °C
Cp  Specific heat capacity  J kg-1 K-1
α  Coefficient of thermal expansion  µm m-1 K-1
ρ  Density  kg m-3
ρel  Resistivity  nΩ m
λ  Thermal conductivity  W m-1 K-1
EC  Electrical conductivity  %IACS
aluSelect: Physical and Elastic Properties